Why trial mixes
Cement, aggregates and temperature all change how an admixture behaves, so the data sheet range is a starting point and not a final dose.
Start with a baseline
Cast a control mix without admixture at the target water-cement ratio and record slump, temperature and density.
Step the dose
Repeat the mix with increasing doses of your superplasticizer, such as SNF / PNS or PCE. Keep the water and cement constant and record slump after mixing.
Check slump over time
Measure slump again at the time concrete would reach site, for example after 30, 60 and 90 minutes, to see slump loss.
Verify strength
Cast cubes or cylinders and test them at the ages your specification requires before you fix the dose.
Record and repeat
Repeat when cement source, aggregate or season changes. Ask us for the data sheet through the quotation page.